Mapendekezo
NOELSONTMMIOX A-160M/A-320M nk.
Anza uundaji
Epoxy iliyorekebishwa ya Alkyd-MIO ya kwanza:
Sehemu A | ||
Epoxy iliyorekebishwa alkyd resin | 20 | 50% katika Xylene |
Kijivu cha oksidi ya chuma cha Micro | 30 | NOELSONTMMIOX A-320M |
Kijazaji cha talc | 5 | |
TIO2 | 3 | Unaweza pia kuchukua nafasi na kuweka alumini au kuchorea rangi. |
Thixatrol ST | 0.5 | |
Sehemu ya B | ||
Epoxy iliyorekebishwa alkyd resin | 35 | 50% katika Xylene |
Mafuta ya kutengenezea 100# | 5.5 | |
Kikausha cha Cobalt, 6% | 0.5 | |
Kupambana na ngozi | 0.5 |
Kitangulizi cha juu cha Epoxy-MIO:
Sehemu A | ||
Bisphenol A resini za epoxy | 14.0 | Epikote 828 (Shell) |
Urea-formaldehyde resini | 1.5 | Plastopal EBS 400 (BASF) |
Pombe ya Butyl | 3.0 | |
Xylene | 6.0 | |
Kijivu cha oksidi ya chuma cha Micro | 37 | NOELSONTMMIOX A-320M |
Zinki phosphate | 15 | NOELSONTMZP 409-3 |
Kijazaji cha talc | 5 | |
TiO2 | 5 | |
Thixatrol ST | 1 | |
Pombe ya Butyl | 2.0 | Imeongezwa baada ya mchanganyiko |
Xylene | 10.5 | Imeongezwa baada ya mchanganyiko |
Sehemu ya B | ||
Kigumu cha resin epoxy | 65 | Cardolite NC 541/90 X |
Resin ya petroli | 35 | |
A/B = 6:1 (kwa uzani) |